Most ejector pin failures are not caused by the pin being too soft. They are caused by the wrong steel for the failure mode the mould actually has: heat, abrasion, or bending load. Pick against the failure mode, and the pin survives.
The three steels, briefly
| Steel | Typical hardness | What it is good at | Where it fails |
|---|---|---|---|
| SKD61 (H13, 1.2344) | through-hardened ≈HRC 50–55; nitrided core ≈HRC 40–45 | Hot strength, toughness, takes nitriding well | Lower wear resistance than high-speed steel |
| SKH51 (M2, 1.3343) | HRC 62–65 | Highest wear resistance, holds a sharp edge | More brittle; small pins can snap under side load |
| SUJ2 (52100, 1.3505) | HRC 60–64 | Good wear resistance at the lowest cost | Loses hardness above roughly 200 °C |
Choose by failure mode
The pin bends or snaps
This is a toughness problem, not a hardness problem. Go to SKD61. It has the highest toughness of the three and tolerates misalignment better. Increasing diameter or shortening the unsupported length usually matters more than the steel — but if you must choose one steel, choose SKD61.
The pin wears at the tip or the side
This is abrasion, and it is almost always caused by filled resin. Glass-filled PA66, PBT and PPS grind the pin like sandpaper. Go to SKH51, or keep SKD61 and add a DLC coating. Nitriding helps less than people expect against glass — the nitride layer is thin and brittle and can flake at the tip.
The pin runs hot
Hot runner drops, engineering resins at 280–320 °C, and long cycle times all soften SUJ2. Go to SKD61. It retains hardness at temperature where bearing steel has already given up.
It is a standard pin in a standard mould, and cost matters
SUJ2 is the right answer. For general-purpose pins in commodity moulds running unfilled resin, SUJ2 gives 90% of the life at a lower price. Buying SKH51 for this application is paying for wear resistance you will never use.
The coating decision
Coatings are usually more effective than upgrading the steel, and cheaper than people assume:
| Coating | Best for | Watch out for |
|---|---|---|
| Nitriding | General wear, moderate temperature | Thin case; can crack at sharp tip radii |
| DLC | Glass-filled resin, low friction, sticky plastic | Needs a good substrate underneath; not for high temperature |
| Hard chrome | Corrosion, release | Environmental restrictions in some markets |
A nitrided SKD61 pin outperforms a plain SKH51 pin in most glass-filled applications, and costs less than moving to a premium steel.
What we actually do
We machine ejector pins from all three steels, hardened to the range you specify, ground to g6 with straightness within 0.01 mm over 100 mm. If you send a drawing without a material, we will ask what the resin is and what the failure mode has been — because the material answer follows from those two facts, not from a preference.
See the full range on the ejector pins page.
Questions
Which steel is best for glass-filled nylon?
SKH51 offers the highest wear resistance, but a nitrided or DLC-coated SKD61 pin usually gives a better balance of toughness and wear and costs less. For small diameter pins in glass-filled resin, coating matters more than the base steel.
Can SUJ2 pins be nitrided?
Yes, but SUJ2 already runs at HRC 60–64, and nitriding adds a thin brittle case that can crack at sharp tip radii. It is usually better to choose SKD61 if you need a nitride case.
What hardness should an ejector pin be?
SKD61 through-hardened ≈HRC 50–55 (nitrided: hard case over a tougher core); SKH51 ≈HRC 58–62; SUJ2 ≈HRC 58–62. Harder is not automatically better — above about HRC 62 the risk of brittle fracture at the head-to-shaft transition rises quickly.
Working on a part like this?
Send a drawing — STEP, IGES, DWG or a photo with dimensions. We reply within one business day with a DFM note and a price. One piece is acceptable for standard sizes.